Precision sheet metal spraying is the process of applying coatings (organic or inorganic) onto the surface of a workpiece using spraying or brushing methods, such as oil spraying and painting.
Traditional painting techniques include brushing, spraying, dipping, and rinsing, as well as high-pressure airless spraying, electrostatic spraying, and electrophoresis, which are widely used.
Electrostatic spraying is divided into electrostatic powder coating and electrostatic spray coating. Electrostatic spraying refers to the process in which atomized paint particles carry negative charges in a direct current voltage of 80-90KV electric field, and uniformly adhere to the positively charged surface of the workpiece under the action of electric field force, forming a paint film.
The advantages of electrostatic fuel injection are obvious. Firstly, it has high production efficiency, good working conditions, and is suitable for large-scale assembly line operations; Secondly, the paint layer has high quality, good adhesion, uniform and smooth paint film; Thirdly, save paint, generally saving 60% compared to manual spray painting. Electrostatic powder coating: Under the dual action of electrostatic force and carrier gas, powder coating is evenly applied to the workpiece. When the powder layer reaches a certain thickness, the “same sex repulsion” principle between the powder layers prevents further powder coating on the workpiece, thus avoiding excessive powder coating on the surface of the workpiece. After a certain period of time and temperature baking, a certain thickness coating is finally formed. The characteristics of powder spraying are basically the same as those of oil spraying, but the utilization rate of powder spraying can reach 99%, and the thickness of a single spray can reach 40-100UM.
1. The quality of sheet metal surface spraying is mainly controlled.
1.1 Spray color and color difference control
There are many factors that affect the color difference of spray painting, which can be mainly summarized as follows:
(1) Differences in raw materials: Different batches of coatings may result in slight variations in pigment composition, leading to color differences. (2) Inconsistencies in spraying process parameters, including the distance, angle, pressure, and dilution ratio of the spray gun, can cause differences in coating thickness and uniformity, leading to color differences. (3) The conditions of the substrate are different: different materials have different abilities to absorb and reflect light, and even with the same coating, color differences may occur on different substrates. (4) The influence of environmental conditions, such as temperature, humidity, and lighting conditions in the spraying workshop, can also affect the dryness and glossiness of the coating during the spraying process, leading to color differences. (5) Human factors: The technical level, experience, and condition of the operators will have a significant impact on the coating effect.
In actual production, the common types of color differences are divided into the following categories: (1) Color difference: refers to the inconsistent color tone expression between two colors, such as one leaning red and the other leaning yellow. (2) Brightness difference: Refers to the degree of brightness and darkness of a color, that is, the difference between dark and light. (3) Poor purity: manifested as differences in the vividness or saturation of colors.
When encountering color differences in spray painting, you can try the following methods: (1) Coating preparation: When encountering color differences, adjust the coating formula to fine tune the color. (2) Process optimization: Fine tuning of spraying process parameters, such as changing spraying pressure and spraying distance. (3) Remedial measures: If the product has already produced color differences, partial spraying or overall re spraying can be carried out to eliminate the differences.
1.2 Coating thickness
According to the national standard “Anti corrosion Coating of Fusion Bonded Epoxy Powder Coatings”, the spraying thickness should be 0.17-0.3 millimeters. The general automatic line is set to 60 microns to 80 microns and can be inspected using a thickness gauge.
1.3 Coating adhesion
The adhesion of coatings includes two aspects: the adhesion between organic coatings and substrate metal surfaces, and the cohesion of organic coatings themselves. The stronger the adhesion strength between organic coatings and metal surfaces, the better. The combination of the tough and dense paint film of the coating itself can better block the corrosion of metals by external corrosion factors, thereby achieving good protection of metals. The coating cannot firmly adhere to the metal surface, and even the best coating is ineffective. The coating itself has poor cohesion, and the paint film is prone to cracking and losing its effectiveness. The above two factors jointly determine the adhesion of the coating and constitute the key factors determining the protective effect of the coating. Testing of coating adhesion: on-site testing and laboratory testing. On site inspection: Use cutting tools to mark X or grid, as well as pull open method. Laboratory testing: Circle drawing method. Scope of application: The X-mark method is used when the dry film thickness is greater than 125m; The grid method is suitable for dry film thickness of 250um.
2. Common testing methods for the quality of precision sheet metal surface spraying.
2.1 Visual Inspection
Visually inspect the color difference, missed spraying, particles and other defects of the sprayed surface layer with the eyes under certain lighting conditions, which is convenient and fast, and can quickly select unqualified products.
2.2 Baige knife inspection
Baige knife uses a certain specification tool to cut and penetrate the coating in a grid pattern. The completed grid pattern is classified into six levels to evaluate the resistance of the coating to separation from the substrate. Mainly applicable for determining the adhesion of organic coatings using the grid cut method. Not only suitable for laboratories, but also for construction sites under various conditions.
2.3 Common inspection equipment and functions for precision sheet metal spraying quality
The commonly used equipment for inspecting spray quality includes: coating thickness gauge, adhesion tester, salt spray test chamber, surface condition detector, and color photometer. These devices can help spray manufacturers to accurately control the quality of spraying, provide precise technical guarantees for spraying work, ensure that the quality of coatings meets design requirements, and improve production efficiency and product quality.
(1) Coating thickness gauge is used to measure the thickness of coatings on the surface of substrates, and it is an essential equipment for quality inspection in spray painting factories. Coating thickness gauges are widely used in fields such as construction, automobiles, ships, and home appliances. By detecting the thickness of the coating, the quality of the coating can be ensured to meet the design requirements, ensuring the service life and performance stability of the product.
(2) Adhesion tester is used to test the adhesion of coatings, that is, the adhesion between coatings and substrates. It can evaluate the firmness of coatings, assess their resistance to peeling, scratching, and chemical stability in different environments. The adhesion tester is suitable for quality inspection in industries such as coatings, paints, steel structures, and chemicals.
(3) Salt spray test chamber is a device that simulates the corrosion effect in natural environments. It can accelerate the aging and corrosion process of coatings in a short period of time, and evaluate the anti-corrosion performance of coatings. The commonly used salt spray test chambers in spray painting factories include tower shaped salt spray test chambers and circular salt spray test chambers. By testing the corrosion resistance of the coating in a salt spray environment, it can be ensured that the quality of the coating meets the design requirements.
(4) Surface condition detector is a device used to evaluate the surface roughness, shape, size, and other aspects of workpieces. It can provide a prerequisite for surface quality for spray painting factories. The surface condition detector can detect the surface condition of any curved surface such as flat, spherical, cylindrical, etc., and measure indicators such as surface accuracy, flatness, and shape accuracy.
(5) Color photometer is a device used to measure parameters such as color and brightness of objects. Spray painting factories need to inspect and adjust colors, and color photometers can quickly and accurately measure the color and brightness values of coatings, providing reference data and precise quality control measures for spray painting factories.
3. Common problems and their causes in spray painting, as well as corresponding solutions.
3.1 Flow hanging
The coating flows from top to bottom on the vertical surface of the object being coated, causing uneven flow marks on the coating film. According to the shape of the flow mark, it can be divided into sinking, hanging, and flowing.
Cause analysis: (1) The solvent used evaporates too slowly or the coating is not compatible. (2) The paint was sprayed too thick at once, and the spraying operation was improper. (3) The ambient temperature is too low or the solvent vapor content in the surrounding air is too high. (4) The viscosity of the coating is low. (5) Coatings contain pigments with high density. (6) Some substrates are prone to sagging.
Solution: (1) Choose the solvent correctly, pay attention to the solubility and volatilization rate of the solvent. (2) To improve the proficiency of workers in spraying operations, the coating thickness should be uniform, and it is not advisable to spray too thick at once. Generally, it is advisable to control it at around 20um. If a coating of 30um to 40um needs to be sprayed at once, the wet touch wet process (applicable to thermosetting coatings) should be used. (3) Strictly control the construction viscosity and environmental temperature of the coating. (4) Strengthen ventilation. (5) When applying new paint on an old coating, it is necessary to polish it first.
3.2 Particles
The phenomenon in which foreign objects appear in particles during coating and are distributed on the entire or partial surface of the coating is called particles. Particles caused by foreign objects mixed into the coating or deterioration of the coating are called particles; The protruding foreign objects caused by aluminum powder in metal flash coatings on the surface of the coating are called metal particles; Dust or foreign matter adhering to the wet film during or just after painting is called dust.
Cause analysis: (1) The cleanliness of the air in the painting environment is poor, such as dust in the paint mixing room, painting room, settling area, and drying room. (2) Coatings that are prone to sedimentation are not thoroughly stirred or the paint skin is mixed in the coating without being filtered and removed. (3) The surface being coated is unclean or there is dust on the operator’s work clothes and gloves. (4) Deterioration of coatings, such as precipitation or coarsening of paint base, poor dispersion or agglomeration of pigments, precipitation of organic pigments, and poor dispersion of aluminum powder in the paint base of glitter colored paints.
Solution: (1) The supply air and dust removal in the paint mixing room, painting room, and static area should be sufficient to ensure a clean painting environment. (2) The paint should be thoroughly mixed and a filter should be installed on the paint supply pipe. (3) The surface of the coated object should be cleaned, for example, by wiping off dust with a sticky cloth or blowing off dust with ionized air. Operators should not wear work clothes and gloves that are easy to fall off during operation.
3.3. Poor exposed and covered bottom
Exposed substrate is caused by overspray, commonly known as lack of paint. Undercover defect refers to the phenomenon where the coating is too thin and exposes the color of the substrate after the coating is dried.
Cause analysis:(1) The composition ratio of paint ingredients is incorrect, such as insufficient amount of pigment, resulting in poor covering ability. (2) The viscosity of the coating application is low, the coating is too thin, or it is not thoroughly stirred before use. (3) The appearance of the coated object is complex, causing some parts to experience leakage.
Solution: (1) Choose coatings with strong covering power. (2) Appropriately increase the viscosity of the coating application, stir thoroughly before use, and ensure that the coating film reaches the specified thickness. (3) For complex coated objects, careful coating is required and no omissions are allowed. (4) Try to use paint with colors similar to the primer and topcoat.
3.4 Pinholes
Create small holes on the coating that resemble needle like punctures or small holes on the surface of leather.
Cause analysis:(1) The viscosity of the coating during construction is too high, resulting in poor leveling and bubble release. (2) Mixing oil and water into the coating causes pinholes on the surface of the coating. (3) The paint deteriorates during storage, transportation, and use. (4) The coating dries quickly, or the coated material is directly baked at high temperatures without being air dried, causing the coating to undergo a rapid polymerization reaction. When the solvent evaporates, it breaks through the surface coating and causes pinholes. (5) The humidity in the painting environment is too high, or there are dirt and small holes on the surface of the coated object.
Solution: (1) Choose appropriate coatings, strengthen inspection of coatings that are prone to pinholes, and strictly follow the process specifications for adjusting the viscosity of coatings. (2) Pay attention to the cleanliness of painting tools, coatings, and diluents to prevent small particles and other impurities from mixing into the coating. (3) Strengthen paint inspection, and do not put unqualified paint into production. (4) Strictly following the process regulations, after painting, it should be dried first and then sent to a high-temperature area for baking. (5) Improve the painting environment, pay attention to the cleanliness of the coating surface, and fundamentally eliminate small holes on the surface.
3.5 Color difference
The phenomenon where the gloss and hue of the coated film after painting differ from the standard sample or the color of the repaired area is different from the original coating.
Cause analysis:(1) There is a significant color difference between the batches of paint used, or when changing colors, the painting tools and equipment are not cleaned thoroughly.
(2) Poor polishing of the repaired area results in uneven gloss.
Solution: (1) Strengthen the inspection of coatings to prevent coatings with large color differences from entering the factory. When changing colors, the painting equipment, tools, and roller paint pipes should be thoroughly cleaned. (2) Try to minimize touch ups, especially local repairs. The repair area should be carefully polished, and the repair area should be expanded as much as possible to the position where there is a clear boundary line on the surface.
3.6 Bubbling
The surface of the dried coating presents tiny bead like bubbles that rupture upon contact and pressure.
Cause analysis: (1) After coating, immediately enter high temperature baking, the surface solvent evaporates immediately and dries into a film, and the internal solvent cannot evaporate in time, causing small bubbles to emerge from the surface coating. (2) Before painting, the surface of the object to be coated is not clean, and water or oil is mixed in the coating or diluent. (3) The coating is too thick or the viscosity of the coating is too high.
Solution: (1) Strictly follow the drying temperature and time requirements for each layer of coating specified in the process, and do not heat up too quickly. (2) Ensure the surface of the coated material is clean and strictly control the mixing of water, oil, etc. into the compressed air used for spraying. (3) The construction viscosity of the coating should comply with the process specifications, and the coating should not be too thick. (4) Alcohol solvents or defoamers can be added to coatings.
3.7 Orange Peel
A wrinkled surface resembling orange peel appears on the coating.
Cause analysis: (1) Excessive viscosity and poor leveling of the coating. (2) The nozzle diameter of the spray gun is too large, the compressed air pressure is insufficient, the atomization effect is poor, and the spraying distance is inappropriate. (3) The wind speed in the spraying room is insufficient, and the drying time is short. (4) Insufficient coating thickness and short drying time. (5) The coated material and ambient temperature are too high.
Solution: (1) Adjust the viscosity of the coating according to the process specifications. The viscosity should be slightly higher at low temperatures and slightly lower at high temperatures. Add leveling agents appropriately to improve the leveling performance of the coating. (2) Adjust the caliber and spraying distance of the nozzle, choose the appropriate compressed air pressure to achieve the best atomization effect. (3) The indoor wind speed should be adjusted to meet the process requirements, and organic solvents with high boiling points and slow volatility should be selected. (4) In the absence of sagging, a single spray should reach the specified thickness and extend the drying time appropriately. It is not advisable to enter the high-temperature drying room too early. (5) The temperature of the coated material should be cooled to below 50 degrees Celsius, and the temperature inside the coating and spraying room should be maintained at around 20 degrees Celsius.
3.8 Cracks in putty
The phenomenon of loss of gloss or intermittent marks on the surface of the coated object that has been scraped with putty.
Cause analysis: (1) Insufficient polishing and high shrinkage of the areas where putty has been scraped, resulting in deformation after curing. (2) The putty layer absorbs paint and is not coated with sealing primer after scraping.
Solution: (1) Choose low shrinkage putty and thoroughly polish the areas where putty is applied. (2) Choose putty with the same color as the bottom layer, and apply paint or intermediate coating after polishing.
3.9 Color fading
After the coating is completely dried, there is a phenomenon of coating coloring on the wiping cloth when wiped clean.
Cause analysis: (1) Mainly caused by the penetration of pigments into the surface of the coating, with organic pigments penetrating more severely.
Solution: (1) Try to use non fading coatings (2) Add paint base or coat the selected coating with gloss.
4. Conclusion
With the change of market environment and the improvement of public quality awareness, product quality has become the most important issue for the survival and development of enterprises. How to produce high-quality products that meet social needs has become a common topic in the entire industry. As a manufacturer integrating precision sheet metal research and production, we have always adhered to the principle of seeking development through reputation and survival through quality. We continuously invest in improving product quality and vigorously conduct research and development. From the design of product appearance and structure to welding and spraying in production, scientific and precise quality control is carried out, striving for excellence. Spray coating process is the most widely used method in precision sheet metal surface treatment. Its function is not limited to beautifying parts and products, but also takes into account many functions such as corrosion resistance, high temperature resistance, and wear resistance. The quality of spraying plays a crucial role in the quality of the product and the customer experience. Surface treatment is often the last process in product production, and if the quality is not well controlled, the entire product may be in vain. Not only will its aesthetic appeal be compromised, but its functionality will also be greatly reduced. Therefore, it is necessary to understand common problems in spraying, analyze the reasons, and find reasonable treatment methods.
Why do “pinholes” or bubbles appear in the finish, and how are they managed?
Pinholes are tiny, needle-like holes that appear in the coating after curing, often compromising both the look and the protective quality of the finish.
The Cause: These are typically caused by trapped gas or moisture. If the metal surface is porous or wasn’t completely dry after the pretreatment phase, moisture can turn to steam during the high-heat curing process and “pop” through the coating. It can also be caused by applying the coating too thick, which traps air underneath.
The Solution: Ensuring that parts are thoroughly dried in a “dry-off” oven after pretreatment and before spraying is essential. Additionally, maintaining a consistent coating thickness—avoiding “heavy” spots—allows any incidental air to escape before the surface skins over.
What leads to “sagging” or “running” in a sprayed finish, and how can it be avoided?
Sagging (often called “curtains” or “tears”) occurs when the applied coating moves under gravity before it has a chance to set or cure.
The Cause: This is usually the result of over-application in a single pass, which makes the wet film too heavy to stay in place. It can also happen if the spray gun is held too close to the metal or if the viscosity of the liquid paint is too low (excessive thinning).
The Solution: The best approach is to apply the coating in multiple, thin, uniform layers rather than one thick coat. Operators should also maintain a consistent distance and speed with the spray gun to ensure an even distribution. For powder coating, ensuring the electrostatic charge is correctly calibrated will help the powder “stick” more uniformly to the part.